Operating a heat treatment kiln for ISPM 15 means loading pallets or lumber so hot air reaches every piece, measuring the core temperature of the thickest components, and holding at least 56 °C at the core for 30 continuous minutes, with every cycle recorded. In practice, success depends on correct probe placement, enough humidity and airflow, calibrated sensors and disciplined record keeping that an inspector can audit at any time.
The requirement in one line
ISPM 15, the international standard for wood packaging material, requires heat treatment (code HT) to raise the wood to a minimum core temperature of 56 °C for at least 30 continuous minutes throughout its whole profile. The standard sets the result, not the equipment: conventional steam or hot-air kilns, kiln drying chambers and other approved heat sources can all be used, as long as the national plant protection organization (NPPO) or its accredited agency has approved the facility and its monitoring method. Background on the treatment itself is in heat treatment (HT) of wood packaging.
Heat treatment is not the same as kiln drying. A heat-treated pallet can still be wet, and a dried board is not automatically treated. See kiln dried vs heat treated.
Monitoring methods and probe placement
Approval schemes generally allow three ways to show that the core reached the target.
| Method | How it works | Typical conditions |
|---|---|---|
| Direct core measurement | Thermocouple probes inserted into the center of the thickest pieces, holes sealed | Most common for pallet kilns |
| Wet/dry bulb schedule | Chamber wet bulb and dry bulb held at validated values for a set time, based on wood thickness | Lumber kilns, validated schedules |
| Dry bulb only | Chamber dry bulb held at a validated temperature for an extended time | Requires verification studies |
The US enforcement regulations of the American Lumber Standard Committee (ALSC), for example, accept direct measurement of the wood core temperature of the thickest piece or pieces, using thermocouples properly sealed with non-conductive material; the number of thermocouples is set during facility qualification or verification studies. Verification studies are required when a chamber runs dry heat below 71 °C (160 °F), or dry and wet heat below 60 °C (140 °F).
Good practice for core probes
- Choose the slowest-heating piece. Use the thickest, densest and wettest components, typically blocks or stringers, not deck boards.
- Drill to the geometric center. The probe tip should sit at the middle of the cross-section and away from the ends, where heat enters faster.
- Seal the hole. Use non-conductive sealant or putty so hot air cannot travel down the hole and give a false high reading.
- Place probes where airflow is weakest. Typical cold spots are the center of the load, the bottom of tall stacks and the side furthest from the fans; validation tests show where they are in each kiln.
- Use enough probes. The minimum is set by the approval scheme; the cycle ends only when the slowest probe has completed its hold time.
Research by NC State University on hardwood pallet parts used a thermocouple placed at the center of the largest component, which is the same principle used in commercial practice.

Wet bulb, dry bulb and why humidity matters
A kiln's dry bulb is the actual air temperature. Its wet bulb is the temperature of a sensor kept wet by a wick; evaporation cools it, so the difference between the two (the wet bulb depression) indicates how dry the air is. Wood surfaces that are still wet tend to stay near the wet bulb temperature, because evaporation absorbs heat.
This has a practical consequence: raising the dry bulb alone does not guarantee fast heating if the air is very dry and the wood is wet. NC State trials found that a steaming schedule (wet bulb 160 °F, about 71 °C) heated gum stringers to the target in about 70 minutes and oak blocks in about 100 minutes, while a dry heat schedule (dry bulb 180 °F, wet bulb 160 °F) needed about 85 and 165 minutes respectively. Higher humidity improves heat transfer and also limits surface checking.
The Canadian Food Inspection Agency's heat treatment program, as another example, requires dry and wet bulb sensors to read within ±2.5 °C, and temperatures to be recorded at least every 30 minutes for schedule-based treatment of lumber.
Cycle times and loading
There is no fixed cycle time; it depends on what is in the chamber.
| Factor | Effect on heating time |
|---|---|
| Thickness of largest component | Strongest effect; heat time rises steeply with thickness |
| Moisture content | Green wood heats more slowly than dry wood |
| Initial wood temperature | Frozen wood in winter needs extra energy and time |
| Species and density | Dense hardwoods heat more slowly |
| Stacking density | Tightly stacked loads block airflow |
| Air velocity and humidity | Higher airflow and humidity speed up heating |
In the NC State trials, dead-piled cants about 6 in (152 mm) thick needed up to 941 minutes, compared with roughly 1–3 hours for stringers and blocks. A 2012 Forest Products Journal study on vacuum-steam treatment reported treatment of hardwood pallets in under 65 minutes and contrasted this with conventional cycles of 2 to 4 hours. Thin assembled pallets in a well-designed kiln are usually at the shorter end; stacks of thick blocks or cants are at the longer end.
Loading rules that shorten cycles and reduce failures:
- Leave air gaps between stacks and between stacks and walls, matching the kiln's airflow direction.
- Avoid mixing very thick and thin components in one charge; the thickest dictates cycle time.
- Do not block fans or baffles; keep doors and seals in good condition.
- Load pallets so air can pass through the entry openings.
Records, calibration and marking
A heat treatment cycle that is not documented does not count. Typical record requirements include:
- date, kiln number, charge number and quantity and type of material;
- probe locations and the temperature curve of every probe;
- start and end of the 30-minute hold, identifying the slowest probe;
- operator signature and any deviations or alarms;
- calibration certificates for probes and recorders.
The ALSC regulations call for annual calibration of temperature monitoring and recording equipment for each chamber in many cases, recalibration when variance exceeds ±2.8 °C (±5 °F), and monthly inspections of wood packaging facilities by the accredited agency. Other countries have similar schemes run by their NPPO. Only material from a completed, documented cycle may receive the ISPM 15 mark with the HT code. See the ISPM 15 mark and how producers get certified.

Energy: heat sources and biomass boilers
Heat treatment is energy-intensive because both the wood and its water must be heated. Common heat sources are:
- Biomass boilers burning the plant's own sawdust, offcuts and ground pallet waste, producing hot water, steam or thermal oil;
- Gas or oil burners, direct or indirect;
- Electric heating, more common in small chambers;
- Waste heat from other processes.
Biomass is popular because pallet plants generate a steady stream of wood residue that otherwise has to be sold or disposed of. Operators should account for local air-emission permits, fuel moisture (wet fuel lowers boiler efficiency) and storage fire risk. Residue use is covered in pallet wood waste as biomass, and kiln types in heat treatment kilns: types and sizing.
Common failures and how to avoid them
- Probe in the wrong piece or position. A probe in a thin board or near an end reads high while the real cold spot is still below target.
- Unsealed probe holes. Hot air channels down the hole and inflates readings.
- Poor airflow. Overloaded chambers, collapsed stickers or failed fans leave cold zones.
- Too-dry air with wet wood. Wood stalls near the wet bulb temperature.
- Power or recorder interruptions. If the record breaks during the hold, the hold must normally restart.
- Uncalibrated sensors. Drift goes unnoticed without regular checks.
- Mould after treatment. Warm, humid pallets stacked tightly and wrapped soon after treatment can develop mould; allow cooling and ventilation. See mould and blue stain.
Frequently asked questions
Does the 30 minutes start when the kiln reaches 56 °C?
No. The 30 minutes count from the moment the core of the slowest-heating piece reaches 56 °C, and the temperature must stay at or above that level for the whole period.
How many probes does a pallet kiln need?
The number is set by the approving agency, usually during facility qualification or verification tests, and depends on chamber size and airflow. The cycle is complete only when every probe has met the requirement.
How long does a typical heat treatment cycle take?
It depends mainly on the thickness and moisture of the largest pieces. Research has reported roughly 1–3 hours for pallet parts and much longer for thick cants; conventional pallet cycles of 2 to 4 hours are commonly cited.
Does heat treatment prevent mould?
No. It kills pests present at the time of treatment but does not make wood resistant to mould. Moisture control after treatment is what prevents mould.
Sources
- Wood Packaging Material Enforcement Regulations (November 2025) — American Lumber Standard Committee
- PI-07: Heat treatment program requirements — Canadian Food Inspection Agency
- Heat Sterilization of Hardwood Pallets and Pallet Material — NC State Extension
- Vacuum-Steam Treatment of Pallets and Pallet Parts for Compliance with ISPM 15 — Forest Products Journal
- ISPM 15 (2009 version) — IPPC